Fabrication of W–1 Wt.% TiC Composites by Spark Plasma Sintering

Xiao-Yu Ding,Lai-Ma Luo,Hong-Yu Chen,Guang-Nan Luo,Xiao-Yong Zhu,Xiang Zan,Ji-Gui Cheng,Yu-Cheng Wu
DOI: https://doi.org/10.1016/j.fusengdes.2015.01.003
IF: 1.905
2015-01-01
Fusion Engineering and Design
Abstract:TiC/W ultra-fine powders were produced by one-step activation and chemical reduction process. The powders were consolidated by spark plasma sintering (SPS) at 1800 degrees C to suppress grain growth during sintering. The grain size, relative density and the Vicker hardness HV0.2 of the bulk sample fabricated by SPS were 3 pm, 98.6% and 471, respectively. The reduced Young's elastic modulus of the sintered W-1 wt.% TiC composites was 382.7 GPa. As the temperature rises from room temperature (RT) to 1100K, the thermal conductivity of pure W and W-1 wt.% TiC composites decreased with the same trend. However, the thermal conductivity of the samples was both above 120 W/m K at RT. (C) 2015 Elsevier B.V. All rights reserved.
What problem does this paper attempt to address?