Preparation of Mg-15%Al-5%Si-0.5%Sb Alloy and Its Microstructure

MA Ying,ZHANG Zhong-ming,XU Chun-jie,SONG Pei-wei,WANG Jin-cheng,GUO Xie-feng
DOI: https://doi.org/10.3969/j.issn.1000-8365.2006.04.017
2006-01-01
Abstract:The master alloys Mg-2.19%Si and Al-17.8%Si and the in-situ composite Mg-15% Al-5% Si-0.5%Sb were prepared by the permanent mould gravity casting. The experimental results show that Mg-2.19%Si master alloy can fabricated by using 4 mm diameter silicon at 810℃, hold for 5hrs under the protection of gas and covering flux. Al-17.8% Si master alloy could be made by the hypothermia silicon adding method. The Sb in the in-situ composite Mg-15% Al-5% Si-0.5% Sb could refine the Mg2Si phase and changedendritic Mg2Si into granular shape, but its refining effect is limited and other measures should be taken to refine structure further.