Abstract:Composite powders were obtained by mixing Fe, C and epoxy resin powders. Green parts were manufactured via selective laser sintering (SLS). After the post processes of degreasing, cold isostatic pressing (CIP), vacuum sintering, hot isostatic pressing (HIP), the relative density and mechanical property were improved. The forming and post processes were discussed, and the microstructures, mechanical properties and density of the mentioned alloys were tested respectively via environmental scanning electron microscope, universal testing machine and archimedes law. The results showed that the final density exceeds 97%, tensile strength exceeds 350 MPa and the elongation is about 9%, microscopic structure is granular pearlite and ferrite.