Abstract:The large particle CeO2 and Y2O3 were prepared using oxalic acid as precipitator. The effects of operational parameters such as stirring velocity, precipitation temperature, feeding speed, aging time, precipitation method, and calcination temperature on particle size and loose density of CeO2 were studied. Under the particular conditions, particle median size of D50 ≥ 30μm, loose density of ≥ 2.0 g/ml of CeO2, and particle median size of D50 ≥ 20 μm of Y2O3 were prepared. This technology had advantages of simple process, less equipment investment, ease of use, and suitability for industrialization products.