Performance Degradation of Lithium‐Ion Batteries with LiNi 0.33 Co 0.33 Mn 0.33 O 2 Cathodes during Long‐Term, High‐Temperature Storage: Behaviors and Mechanism

Zheng Wang,Peipei Pang,Zhen Ma,Hongyu Chen,Junmin Nan
DOI: https://doi.org/10.1002/celc.202001553
IF: 4
2021-01-18
ChemElectroChem
Abstract:The behaviors and mechanism for the performance degradation of 18650 cylindrical lithium‐ion batteries (LIBs) with LiNi0.33Co0.33Mn0.33O2 cathode under the long‐term high temperature (HT) of 80 oC are investigated to insight the safe use of LIBs. It is indicated that the direct current resistance (DCR) increases sharply within 240 h and slows down gradually, while the recoverable capacity (RC) fading and the open‐circuit voltage (OCV) are relatively stable in the initial 240 h and speed up from 240 h to 720 h. With the aid of the analysis of the anode, cathode and separator materials in the batteries stored at 80 oC for 0 h, 240 h, 480 h, and 720 h, the mechanism of the performance‐degradation of batteries is elucidated. It is pointed out that the DCR rise is mainly caused by the anode materials peeling off from the copper foil and the subsequent interface resistance increase. The RC fading is attributed to the partial break of the cathode structure due to the dissolution of transition metal ions (Ni2+, Co3+, and Mn4+), and the dissolution becomes more severe as the time extending. And the separator is suffering a combination of stretching, squeezing, oxidation, and destructed, resulting in internal short circuit and sharp OCV drop, as well as the potential safety risks of LIBs. These results are valuable to establish the accelerated test method to evaluate the batteries in a short time range and advance the safe use of LIBs under high‐temperature.
electrochemistry
What problem does this paper attempt to address?
This paper aims to study the performance degradation behavior and mechanisms of 18650 cylindrical lithium-ion batteries (LIBs) with LiNi0.33Co0.33Mn0.33O2 cathode material under long-term storage conditions at high temperature (80°C). Specifically, the paper focuses on the following aspects: 1. **Direct Current Resistance (DCR) Changes**: - DCR increases sharply within the initial 240 hours and then gradually slows down. - The reason is that the anode material peels off from the copper foil, leading to an increase in interface resistance. 2. **Recoverable Capacity (RC) Decay**: - Relatively stable within the first 240 hours, then begins to accelerate. - This is mainly due to partial rupture of the cathode structure and intensified dissolution of transition metal ions (such as Ni2+, Co3+, Mn4+). 3. **Open Circuit Voltage (OCV) Decline**: - Relatively stable within the first 240 hours, then rapidly declines. - This is because the separator is stretched, compressed, oxidized, and damaged, leading to internal short circuits and potential safety risks. By analyzing the anode, cathode, and separator materials at different storage times (0 hours, 240 hours, 480 hours, and 720 hours), the paper reveals the specific reasons for these changes and proposes corresponding mechanisms. These results are significant for establishing accelerated testing methods to evaluate battery performance in a short time and improving the safe use of LIBs under high-temperature storage conditions.