Cause analysis of fractured 40 Mn steel chain and counter measures

Jinying Song,Xiangyu Qi,Liansheng Chen,Yaqiang Tian,Jianyang Zhang
DOI: https://doi.org/10.13251/j.issn.0254-6051.2015.09.046
2015-01-01
Abstract:Cause analysis on the fracture of 40Mn steel chain was carried out by means of hardness tester, optical microscopy, SEM and EDS, and the counter measures for the fracture was put forward.The results show that following causes leading to the fracture of the chain, i.e.the existence of a large number of non-metallic inclusions, serious banded structure in the hot-rolled plate, surface decarburization and insufficient cooling rate during quenching process.And for different causes of the fractured steel chain, corresponding improvement measures such as optimizing steelmaking process, continuous casting, heating and cooling during the quenching process can be taken, which are effective to avoid the fracture chain and improve the percentage of pass.