Mechanical Properties of a Bulk Cu0.5NiAlCoCrFeSi Glassy Alloy in 288°C High-Purity Water

YY Chen,UT Hong,JW Yeh,HC Shih
DOI: https://doi.org/10.1063/1.2159090
IF: 4
2005-01-01
Applied Physics Letters
Abstract:The tensile properties and fatigue lives of a bulk Cu0.5NiAlCoCrFeSi glassy alloy were measured in 288°C water and compared with those obtained in air at ∼25°C. The bulk glassy alloy retained good tensile properties in 288°C water, i.e., tensile fracture strength and tensile fracture elongation were, respectively, 2660MPa and 2.01% in air and a little lower, 2000MPa and 1.49%, in 288°C water. The results of fatigue tests confirmed the significant decrease in fatigue life in high-temperature water. A decrease in strain rate from 0.5to0.001%s−1 decreased fatigue life by a factor of ∼5.
What problem does this paper attempt to address?