Hot deformation behavior of as-Cast AZ61 magnesium alloy

Zhongxue Feng,Qingnan Shi,Fusheng Pan.,Jun Tan,Liangwei Chen,Xiliang Chen
DOI: https://doi.org/10.4028/www.scientific.net/AMR.750-752.574
2013-01-01
Abstract:Thermal compression tests of AZ61 magnesium alloy were performed at deformation temperature 25-400 degrees C with strain rates ranged from 0.02 to 20 s-1, and the microstructure was studied. The conventional dynamic recrystallization (DRX) and shear zones were observed on grain boundaries at temperatures above 200 degrees C. The shear zone and the temperature rise are considered to be responsible for the fracture of specimens. For the large internal stress concentration in the shear zones and the deformation incompatibility between matrix and shear zones, the fracture grew along with the shear zones and the failure occurred in the large deformation field of the matrix at the high strain rate 20 s-1 even at 400 degrees C.