Abstract:Calcium sulfate whiskers were prepared by hydrothermal method with natural gypsum as raw material.Through SEM as the direct analysis method,optimum process conditions of calcium sulfate whiskers were obtianed as follows:reaction temperature was 130 ℃,initial pH of CaSO4 ·2H2O slurry was 10.0,mass fraction of slurry was 5%,material size was lower than 122 μm,and reaction time was 1.5 h.Under these conditions calcium sulphate whisker product with average diameter of 1.32 μm and L/D ratio of 76~90 was obtained.Pilot test results indicated that L/D ratio and diameter of calcium sulfate whiskers with natural gypsum as raw material was equivalent to the products with pure gypsum as raw material.Conclusion drawn from the experiment will play an important guiding role in the industrial production of calcium sulfate whiskers.