Influence of activator type on reaction kinetics, setting time, and compressive strength of alkali-activated mineral wools

J. Yliniemi,B. Walkley,J. L. Provis,P. Kinnunen,M. Illikainen
DOI: https://doi.org/10.1007/s10973-020-09651-6
IF: 4.755
2020-04-08
Journal of Thermal Analysis and Calorimetry
Abstract:Abstract Alkali activation is a promising utilisation route for mineral wool wastes, due to suitable chemical composition, high reactivity, and surface area. One key factor in the development of alkali-activated binders is the selection of the suitable alkali activator. Here, the effect of sodium hydroxide, sodium silicate, sodium aluminate, and sodium carbonate solution on the alkali-activation kinetics of two main types of mineral wools, stone wool and glass wool, is investigated. Setting time and compressive strength development results are presented, which are explained and discussed in the context of isothermal calorimeter data obtained at temperature of 40 °C. Sodium hydroxide and sodium silicate solutions provided fast reaction with both mineral wools, evidenced by high heat release, high early strength, and fast setting. The reaction with sodium aluminate solution took several days to initiate, but it produced high compressive strength after 28 days of curing with both mineral wools. Glass wool reacted and hardened rapidly with sodium carbonate solution, but stone wool reacted slowly with sodium carbonate and exhibited a low extent of reaction, likely due to lower extent of reaction of stone wool under less alkaline conditions. These results show that mineral wool alkali activation kinetics and binder gel formation are controlled by the activator type and highlight the importance of choosing the most appropriate activator for each desired application.
chemistry, physical, analytical,thermodynamics
What problem does this paper attempt to address?
The problem that this paper attempts to solve is to explore the effects of different alkaline activators on the alkali - activation reaction kinetics, setting time and compressive strength development of mineral wool (including asbestos and glass wool). Specifically, the research aims to optimize the utilization of mineral wool waste by selecting appropriate alkaline activators to develop alkali - activated binding materials with excellent properties. Four different activators were investigated in the study: sodium hydroxide (NaOH), sodium silicate (Na₂O·2SiO₂), sodium aluminate (2Na₂O·Al₂O₃) and sodium carbonate (Na₂CO₃), and their activation effects on the two main types of mineral wool (asbestos and glass wool) were analyzed. ### Main research questions: 1. **Reaction kinetics**: The influence of different activators on the reaction rate during the alkali - activation process of mineral wool. 2. **Setting time**: The influence of different activators on the setting time after the alkali - activation of mineral wool. 3. **Compressive strength development**: The long - term influence of different activators on the compressive strength development after the alkali - activation of mineral wool. ### Research background: - **Utilization of mineral wool waste**: Mineral wool waste is an under - utilized mineral waste with a high specific surface area and good chemical reactivity, which is suitable for preparing alkali - activated binding materials. - **Advantages of alkali - activated binding materials**: Compared with traditional Portland cement, alkali - activated binding materials have higher sustainability and environmental - friendliness. - **Selection of activators**: The selection of activators plays a crucial role in the reaction kinetics, setting time and compressive strength development during the alkali - activation process. ### Research methods: - **Sample preparation**: Mineral wool samples without added organic resins or other additives were collected and ground. - **Activator preparation**: Solutions of different concentrations of NaOH, Na₂O·2SiO₂, 2Na₂O·Al₂O₃ and Na₂CO₃ were prepared. - **Experimental methods**: The heat flow of reaction was measured by isothermal calorimetry, the setting time was determined by using a Vicat device, and the compressive strength was determined by compression tests. ### Research results: - **Reaction kinetics**: The NaOH and Na₂O·2SiO₂ solutions react rapidly with mineral wool, showing high heat release and early high strength. While the 2Na₂O·Al₂O₃ solution reacts more slowly, but can reach a relatively high compressive strength after 28 days. - **Setting time**: The asbestos activated by NaOH has the shortest setting time (3 hours), while the asbestos activated by Na₂CO₃ has the longest setting time (30 hours). For glass wool, the Na₂CO₃ and Na₂O·2SiO₂ activators show a relatively fast setting time. - **Compressive strength development**: The asbestos activated by NaOH reaches a compressive strength of 20 MPa within 1 day, while the asbestos activated by 2Na₂O·Al₂O₃ reaches the highest compressive strength of 59 MPa within 28 days. Glass wool shows good compressive strength under all activators, but the glass wool activated by Na₂O·2SiO₂ has a relatively low compressive strength within 1 day. ### Conclusions: - **Selection of activators**: The type of activator has a significant impact on the alkali - activation reaction kinetics, setting time and compressive strength development of mineral wool. Selecting an appropriate activator can significantly improve the utilization efficiency and performance of mineral wool waste. - **Environmental impact**: From an environmental perspective, the NaOH and Na₂CO₃ activators have lower carbon emissions and are more suitable for use in sustainable building materials. Through these studies, the paper provides important scientific basis and technical support for the effective utilization of mineral wool waste.