Abstract:Based on thermodynamic theory analysis, atmospheric pressure hydrochloric acid leaching method was used to extract nickel and cobalt from laterite, and the dissolution mechanism of valuable metals was discussed. The results show that, with the initial acid concentration of 8 mol/L, leaching temperature of 360 K, solid/liquid ratio at 1∶4, and reaction time of 2 h, the leaching rates of Ni, Co, Mn attained 94%, 61%and 96%, while the leaching rates for Fe and Mg reached 56% and 94%, respectively. According to the thermodynamic calculation and leaching mechanism analysis, the dissolution order for the main minerals amid the laterite leaching is sequentially as follows: goethite followed by lizardite, magnetite and hematite.