Preparation of Low Sulfur Expanded Graphite from Natural Fine Graphite by Microwave

Lang Qin,Xiuyun Chuan
DOI: https://doi.org/10.3969/j.issn.1000-8098.2014.01.001
2014-01-01
Abstract:Using average particle size of 20~30μm natural lfake graphite as raw materials, intercalation agent concentrated nitric acid, potassium permanganate, phosphorus pentoxide as the oxidant, the use of strong acid impregnation method oxidation preparation of expandable graphite intercalation after the microwave method, expanded graphite is gotten. Study the impact of the ifne lfake graphite intercalation and expansion of the main factors to determine the best conditions for the preparation of expanded graphite:graphite, potassium permanganate and phosphorus pentoxide mass ratio of 20∶7∶25, nitric acid concentration of 68%, the reaction time of 80 min, the reaction temperature 25℃, a microwave power of 800 W, the microwave time is 20 s, the maxmium expansion volume of 25.0 mL/g can be obtained.