Abstract:The welding of FGH96/GH4169 superalloy was carried out by using inertia friction welding machine. After welding, the microstructure, microhardness, mechanical properties and fracture morphology of the joint were studied by using optical microscope, SEM and tensile testing machine. The results show that the microstructure of weld zone consists of refined and equiaxed grains, the grains of thermo-mechanically affected zone are stretched to streamline. The tensile strength at room temperature of the joint is close to 80% of that of the base metal. The microhardness distribution shows W shape along the direction perpendicular to the weld, and the lowest hardness is in TMAZ at the GH4169 side. The fracture is also located in the region, and the fracture mode is ductile fracture.