Abstract:Throung tests of non-destructive detection, analysis of chemical composition, metallurgy, energy spectrum, and fractures for the failed reinforcing wires of incoming gas safety isolating strainer on gas turbine No.3 in Yueliangwan Gas Tubine Power Plant, it is determined that one cause leading to early fracture is unsuitable proportion of alloy composition for the stainless wires, the content of mangonese being high, eduction of intergranular carbide, as well as sirious quality problems existing in the material used. It is recommended to select OOCr 17 Ni14 Mo3 or 316L (OOCr17N:14MoZ) austenitic stainless steel having ultta-low carbon content, high Cr and Ni content, and 2%~3%Mo content, and the fabrication of reinforcing wires having to be in conformity with requirements of standard GB4240.