Dielectric and piezoelectric properties of BiScO;-Bi(Zn;Ti;)O;-PbTiO; high Curie temperature ceramics

zhang qiang,li zhenrong
2016-01-01
Abstract:(1-x)Bi(Sc;(Zn;Ti;);)O;-xPbTiO;(BS-0.1BZT-xPT)ceramics were prepared by conventional powder-processing method.It is found that the lattice structure gradually changes from rhombohedral phase to tetragonal phase with increasing the PT content,and the PT content between 0.60 and 0.62 is the phase transitional region between the rhombohedral phase to the tetragonal phase.When PT content is 0.6,the samples exhibited good piezoelectric properties with d33 about 250pC/N and kpabout 43%.With increasing the PT content,the Curie temperature(Tc)is increased,and the value ofεr maxis first increased and then decreased.Finally,it can be found that,when PT content is 0.6,the samples also exhibit good ferroelectric properties with Pr=34.4μC/cm; and Ec=19.2kV/cm.