Abstract:The anodic polarization potential, corrosion rate, surface product after polarization and microstructure before and after polarization of Pb-0.3%Ag-0.03%Ca-0.03%Sr quaternary anode for electrowinning of zinc were studied and compared with Pb-1%Ag ternary anode. The results show that the anode steady potential of Pb-1%Ag and Pb-0.3%Ag-0.03%Ca-0.03%Sr are 1.835 V and 1.875 V, respectively, while the corrosion rate is 57 mg/(m 2 ·h) and 104 mg/(m 2 ·h). The surface structure after experiment in Pb-1%Ag anodes is dense and tightly attached to the base, the phases of the surface are α-PbO2, β-PbO2, PbSO4, Pb and Ag2SO4. While the surface of Pb-0.3%Ag-0.03%Ca-0.03%Sr is loose and like squama, the phases of the surface are α-PbO2, β-PbO2, PbSO4 and PbO1.57.