Study on Semi-Solid Billet Prepared by SIMA Method

韩飞,于霄,王卫卫
DOI: https://doi.org/10.3969/j.issn.1000-3940.2008.06.017
2008-01-01
Abstract:SIMA was adopted to make semi-solid billet.7A09 cast ingot of Ф33 mm×15 mm was used to make billet by direct extrusion and isothermal treatment.The billet was observed by metallographic method in order to determine the parameters for making the semi-solid billet.The main factors in this experiment were extrusion ratio,isothermal temperature and holding time.The results show that the preferred values are extrusion ratio of 7,mould temperature of 300 ℃,cast condition sample's heating temperature of 450 ℃ and holding for 30 min and lower extrusion velocity in the process of billet pretreatment.In the process of isothermal treatment,heating temperature of 617 ℃ and holding for 19 min can acquire perfect semi-solid microstructure.