The effects of Vanadium on the strength of a bcc Fe Σ3(111)[1-10] grain boundary

Sungho Kim,Seong-Gon Kim,Mark F. Horstemeyer,Hongjoo Rhee
DOI: https://doi.org/10.48550/arXiv.1201.5915
2012-01-28
Abstract:The effects of micro-alloying element, vanadium, on a bcc Fe \Sigma 3(111)[1-10] symmetric tilt grain boundary strength are studied using density functional theory calculations. The lowest energy configuration of the grain boundary structure are obtained from the first-principles calculations. The substitutional and interstitial point defect formation energies of vanadium in the grain boundary are compared. The substitutional defect is prefered to interstitial one. The segregation energies of vanadium onto the grain boundary and its fractured surfaces are computed. The cohesive energy calculation of the grain boundary with and without vanadium show that vanadium strengthen the bcc iron \Sigma 3(111)[1-10] grain boundary.
Materials Science
What problem does this paper attempt to address?
The problem that this paper attempts to solve is: the influence of vanadium (Vanadium, V), as a micro - alloying element, on the strength of the body - centered cubic iron (bcc Fe) Σ3(111)[1̄10] symmetric tilt grain boundary. Specifically, the author studied the following problems through density functional theory (DFT) calculations: 1. **Optimal configuration of vanadium at the grain boundary**: - Calculated the lowest - energy configuration of vanadium in the bcc Fe Σ3(111)[1̄10] grain boundary. - Compared the formation energies of substitutional and interstitial sites of vanadium in the grain boundary. 2. **Segregation energy of vanadium at the grain boundary and fracture surface**: - Calculated the segregation energy of vanadium at the grain boundary and on the fracture surface. - Studied the influence of vanadium atom segregation on the grain boundary on its cohesive energy. 3. **Influence of vanadium on grain boundary strength**: - Evaluated the strengthening effect of vanadium on the grain boundary strength by calculating the grain boundary cohesive energy with and without vanadium. ### Specific problems and their solutions - **Selection of substitutional and interstitial sites**: - Calculated the formation energies of substitutional and interstitial sites of vanadium in the grain boundary and found that the energy of the substitutional site is lower, indicating that substitutional defects are more common than interstitial defects. - \[ E_{\text{formation, substitutional}}=- 6.08 \, \text{eV} \quad (\text{relative to isolated vanadium atoms}) \] - \[ E_{\text{formation, interstitial}}=- 4.20 \, \text{eV} \quad (\text{relative to isolated vanadium atoms}) \] - **Calculation of segregation energy**: - Calculated the segregation energy of vanadium from the bulk phase to the grain boundary, and the results showed that the segregation process is exothermic. - \[ E_{\text{segregation}}=- 0.03 \, \text{eV} \] - **Change in cohesive energy**: - Calculated the grain boundary cohesive energy with and without vanadium and found that the presence of vanadium enhances the grain boundary cohesive energy. - \[ \gamma_{\text{coh}} = 1.43 \, \text{eV} \quad (\text{without vanadium}) \] - \[ \gamma_{\text{coh}}^{\text{seg}} = 1.54 \, \text{eV} \quad (\text{with vanadium}) \] - The enhancement amount is: - \[ \Delta \gamma_{\text{coh}} = 0.11 \, \text{eV} \] ### Conclusion Through DFT calculations, the research shows that vanadium mainly exists in the form of substitutional defects in the grain boundary, and the segregation of vanadium significantly enhances the cohesive energy of the bcc Fe Σ3(111)[1̄10] grain boundary, thereby increasing the strength of the grain boundary and preventing brittle fracture. This finding is of great significance for understanding how micro - alloying elements affect the microstructure and macroscopic properties of steel materials.