Differences in mechanical properties and high temperature deformation behavior between TiBw/Ti65 and TiBw/TA15 composites with network structure

Zhenlun Li,Yuqing Chen,Qingxin Kang,Xunhu Xv,Tongxv Zhou,Guofeng Wang
DOI: https://doi.org/10.1016/j.jmrt.2023.09.216
IF: 6.267
2023-09-01
Journal of Materials Research and Technology
Abstract:In this paper, the differences in mechanical properties and high temperature (HT) deformation behavior between TiBw/Ti65 and TiBw/TA15 composites with network structure were studied. The alloy element distribution and microstructure of TiBw/Ti65 and TiBw/TA15 composites were characterized by the electron probe micro analyzer and transmission electron microscopy. The microstructure evolution during HT deformation was analyzed by electron back scatter diffraction. The mechanical properties of two composites were tested at room temperature and 600–750 °C. Arrhenius and artificial neural network models were developed to predict the peak stress and flow stress, respectively. The results show that the multiple alloying elements and silicide in TiBw/Ti65 refined the grains. TiBw/Ti65 composites had higher deformation activation energy and higher strength under the same deformation conditions. Based on the analysis of differences in microstructure, the strengthening mechanisms of TiBw/Ti65 compared to TiBw/TA15 was mainly from fine grain strengthening, dislocation density strengthening, and Orowan strengthening of silicide. The initial recrystallization temperatures for TiBw/TA15 and TiBw/Ti65 were 700 °C and 750 °C with strain rate of 0.001 s−1, respectively. The above results show that TiBw/Ti65 had better HT deformation resistance.
materials science, multidisciplinary,metallurgy & metallurgical engineering
What problem does this paper attempt to address?
The problem that this paper attempts to solve is to explore the differences in mechanical properties and high - temperature deformation behaviors between TiBw/Ti65 and TiBw/TA15 composites with network structures. Specifically, the research focuses on key parameters such as the differences in mechanical properties of the two composites under different temperature conditions, the distribution of alloy elements and microstructural characteristics, the microstructural evolution during high - temperature deformation, and the recrystallization temperature. Through these studies, it aims to deeply understand the influence mechanism of alloy element composition and distribution on the mechanical properties and microstructural evolution of near - α titanium - matrix composites (near - α TMCs), especially the influence mechanism of silicides on mechanical properties, thereby providing theoretical basis and data support for the design and application of near - α TMCs with higher service temperatures. It is mentioned in the paper that by adding multiple alloy elements (such as Nb, W) and silicides, the TiBw/Ti65 composite exhibits finer grains, higher deformation activation energy and higher strength compared with the TiBw/TA15 composite. In addition, the initial recrystallization temperature of the TiBw/Ti65 composite is also higher than that of the TiBw/TA15 composite, indicating that the TiBw/Ti65 composite has better high - temperature deformation resistance. These results are of great significance for the development of new structural materials suitable for high - service - temperature environments such as high - speed aircraft.