Diffusion Bonding of Hydrogenated Ti6Al4V Alloy Containing 0.15 Wt.% Hydrogen

LIU Hong,FENG Jicai,HE Peng
DOI: https://doi.org/10.3321/j.issn:0253-360x.2007.03.025
2007-01-01
Abstract:The diffusion bonding of hydrogenated Ti6Al4V alloy containing 0.15 wt.% hydrogen was carried out,and the phase component of before and after welding,interface structure and the diffusion holes were investigated by means of scanning electron microscope,electron probe microanalysis and X-ray diffraction.The results showed the phase component of before welding was black strip α plus lamellar(α+βH),and the after was equiaxed α plus the coarse lamellar(α+β) plus hexagonal close packed α′ in the β phase.The diffusion of Al and V in α and βH took place during bonding.With the diffusion bonding parameters increasing,the diffusion holes gradually decreased.When bonded at 850 ℃ for 60 min under a pressure of 12 MPa,the diffusion holes disappeared and the shear strength of the joint was up to 543 MPa.
What problem does this paper attempt to address?