Influence of Heat-Treatment and Element Doping on Critical Current Density of MgB_2/Fe/Cu Wires Fabricated by in-Situ PIT Technique

Wang Qingyang,Zhang Pingxiang,Yan Guo
2007-01-01
Rare Metal Materials and Engineering
Abstract:Ti,Zr-doped dense MgB2/Fe/Cu wires were successfully fabricated adopting the in-situ powder-in-tube (PIT) method using low carbon steel sheath. The short samples wires were sintered at 650~850 ℃ for 2~5 h in argon. Critical current density (Jc) of the wires was measured at 4.2 K in the magnetic field up to 8 T by standard four probe method. High Jc values of 2.1×105A/cm2 were obtained in 3 T at 4.2 K for MgB2/Fe/Cu wires. Mg0.9Zr0.1B2/Fe/Cu wires sintered at 800 ℃ heat the highest Jc. The microstructure observation for wires showed that MgB2/Fe/Cu wires have better grain connectivity and higher density compared to MgB2 bulk samples. The Jc can be further improved to meet the requirement for applications by optimizing the process conditions.
What problem does this paper attempt to address?