Preparation of LiNi0.9Co0.1O2 Material and Study on Its Electrochemical Performance

王新,陈忠,廖代伟
DOI: https://doi.org/10.3969/j.issn.1008-7923.2009.02.010
2009-01-01
Abstract:It is a success for using both doping and changing precursor to improve the traditional cathode material LiNiO2 which is using 10%wt Co doped in the β-NiOOH as the precursor, then solid- phase Sintering with LiOH·H2O in the air. By orthogonal methods we optimize the best sintering temperature is 600 ℃ and sintering time is 24 h for synthesis of the LiNi0.9Co0.1O2; Under these conditions, the first charge and discharge efficiency can be as high as 86%, discharge capacity is to be 167 mAh/g after 20 cycles reversible, and the capacity rates can maintain as high as 94%.