A Study on the Galvanic Corrosion Behavior of Aluminum Bottom Cover with Tin

赵宇晖,宋莉华,李众,孙诗林,王海杰,王佳
DOI: https://doi.org/10.3969/j.issn.1008-7818.2012.10.013
2012-01-01
Abstract:The steady-state polarization curves,galvanic current and galvanic potential determination was used to evaluate of the power of galvanic corrosion tendency of aluminum the bottom cover with tin in acidic beverages in this paper.The results showed that:Sn-Al galvanic potential was far less than 200mV in the seal the deaerator acidic beverages solution,and Sn was the anode,Al was cathode,weak even corrosion behavior,combined with aluminum as cathode,and aluminum rendered in the passive state.Therefore,in the state of the acidic beverage cans,corrosion electrochemical behavior still tinplate corrosion process-based,it can be ignore the aluminum tank tinplate bottom and the possibility of occurrence of severe local galvanic corrosion.