Abstract:Urea formaldehyde resins adhesive was prepared by adopt alkali-acid-alkali technology,subdivision control temperature,addition urea in batches and modification with PVA.The effects of the molar ratio of F/U,reaction temperature,reaction time and PVA addition amount on the content of formaldehyde of adhesive liquid and the shear strength of sample were studied.The results indicated that when the molar ratio of F/U was 1.4:1,the reaction temperature was 95℃,reaction time was 70min,and PVA addition amount was 1.0%,the free formaldehyde content of synthesized urea formaldehyde resin would be less than 0.1% and the shear strength of sample was more than 3.0MPa.