Preparation of Β-Wollastonite Glass-ceramics from Potash Feldspar Tailings

徐景春,马鸿文,杨静,李金洪
DOI: https://doi.org/10.3321/j.issn:0454-5648.2003.02.014
2003-01-01
Abstract:Sintering slag glass_ceramics was prepared by using at mass ratio of potash feldspar tailings(72%) from Shaxian of Fujian province, calcium carbonate(22.7%), and zinc oxide (5.3%), the glass was melted at 1 250 ℃ for 3 h. It is found that zinc oxide was a effective flux agent. The melted glass was quenched in water, and got the glass particles with grain sizes in the range between 0.45 to 0.9 mm. By orthogonal experiments of heating treatments, the glass-ceramics were made from the optimum condition: nucleating at 975 ℃ for 45 min, and crystallizing at 1 100 ℃ for 30 min. The prepared glass_ceramics consists of matrix glass and β _wollastonite crystals with grain size around 2 μm, which has a Vickers hardness of 9.77 GPa.