Investigation Of Infrared Properties Of Lithium-Intercalated Vanadium Pentoxide Films

Gm Wu,Yg Wu,Xy Ni,Z Zhou,Hq Zhang,Zm Jin,X Wu
DOI: https://doi.org/10.1117/12.300708
1998-01-01
Abstract:Vanadium pentoxide films were prepared by evaporation followed by annealing posttreatment in O-2 atmosphere. Lithium was inserted electrochemically from an electrolyde into vanadium pentoxide films so that LixV2O5 was formed. The structure of the posttreated samples was determined by XRD and infrared reflectance was measured by FTIR for as-grown and lithiated films, respectively. The experimental results have shown that V2O5 thin films have some infrared absorption peaks located at 982, 824, 527 and 504 cm(-1), and the infrared vibration bands corresponding to the peaks have a good agreement with the analysis by Abello et al. for polycrystalline V2O5, and there is a obvious influence of lithium insertion on the infrared vibration properties which may be reconciled with the lattice change such as expansion and contraction.